Bosch Process Tutorial: Part 4. Loading and Microloading Effects in Si DRIE
The loading effect and the microloading effect are common phenomena observed not only in deep Si etching but also in conventional Reactive Ion Etching (RIE), and are a barrier to achieving a depth uniformity in etching processes. These two effects strongly appear in the Bosch process (silicon deep reactive ion etching), which is mainly composed of fluorine radical etching. The loading effect is caused by the difference in the consumption rate of fluorine radicals as the etchants. The microloading effect is caused by the difference in the numbers of fluorine radicals transported in narrow spaces (Ex. trenches and holes with a high aspect ratio). Samco processes suppress these two effects and can control the etching depth and achieve excellent uniformity. In addition, the method of microloading effect suppressing can be applied to flattened bottom surface process, which we call the “flat bottom process”.
Loading effect
The loading effect is a phenomenon in which the etch rate change depending on Si aperture (unmasked area) ratios. On the surface of Si, the fluorine radicals are consumed and the by-product, SiF4, is increased. Therefore, a larger aperture ratio of Si area has less fluorine radicals, and the etching rate becomes lower. A typical example is that bare Si wafers show slower etch rates at the center where the Si is exposed to a higher density than at the outer periphery.
Figure 1 shows the etching rate dependency on the aperture ratio of an ø8 inch Si wafer. The etch rate is 40 μm / min at an aperture ratio of 1% and goes to 15 μm / min when the aperture ratio is above 40%.
The loading effect is most noticeable when the sample includes both sparse and dense mask patterns, as shown in Figure 2a. In this case, there are two ways of tackling the loading effect issue. The first is to reduce the process pressure and promote gas diffusion. Figure 2b shows the relationship between the process pressure and the difference in depth between Depth 1 (sparse mask pattern) and Depth 2 (dense mask pattern) in Figure 2a. You can see that at lower process pressure, there is a smaller difference in depth. However, by lowering the pressure, the etch rate is also decreased. The second method is to create a dummy pattern on the wafer to reduce the density difference of the mask pattern.
Microloading effect
The microloading effect is a phenomenon in which fewer fluorine radicals transport the bottom of narrow gaps, causing the etch rate to decrease depending on pattern width. This phenomenon is also known as the RIE lag effect or ARDE (aspect ratio dependent etching). Figure 3 is an SEM image of the microloading effect after Si deep reactive ion etching.
When a pattern has a wide opening (right side of Fig. 3), fluorine radicals transport the bottom of trenches and holes easily, and can be processed at a high Si etch rate. However, when the pattern opening narrows (left side of Fig. 3), the etch rate gradually decreases with the number of fluorine radicals that are able to transport the bottom of the trench or hole. On the other hand, when processing pillar structures, the pattern width has little effect on the etch rate because the flow of fluorine radicals is not obstructed. In the case of trench and hole etching, it is more difficult for fluorine radicals to transport the bottom of patterns with high aspect ratios. This tendency is especially noticeable when etching holes, because radicals are obstructed independently of the direction from which they enter. This is unlike trenches, where radicals are less restricted when moving along the trench line. The rounded bottom seen in Fig. 3 is also due to side walls blocking the flow of fluorine radicals, which increases the ratio of radicals etching the center of the pattern.
Figure 4 shows SEM images of a narrow trench (10 μm) and a wide trench (200 μm) connecting. When a wide trench pattern intersects a narrow trench pattern, fluorine radicals are able to flow from the wider area, increasing the etch rate thus achieving a higher aspect ratio than would be the case for a pattern of only narrow trenches. However, due to the flow of fluorine radicals from the wider area, scallops will form diagonally instead of horizontally. Comb-shaped MEMS devices are another example of patterns with a mixture of narrow and wide trenches. For comb-shaped MEMS devices on SOI (Silicon on Insulator) wafers, even with relatively high aspect ratios, it is possible to etch through to the insulating layer.
Method for suppressing microloading effect
Figure 5 compares the normal Bosch process with Samco’s method for suppressing the microloading effect. The normal Bosch process etches all of the passivation film on the bottom of the trench. Then, in the Si etching step, the etch rate is higher at the bottom of the wider pattern, especially in the center where fluorine radicals are more easily transported. As a result, depth uniformity worsens.
To suppress the microloading effect, some process conditions, such as the pressure during the deposition step, must be adjusted. In the etch step, the difference in the thickness of the deposited film and the difference in the etch rate are balanced and cancel each other out, achieving total depth uniformity. The microloading effect can then be suppressed by optimizing the duration of film deposition and etching for all pattern widths. Figure 6 shows the result of adjusting the process conditions to control the microloading effect.
To suppress the microloading effect, some process conditions, such as the pressure during the deposition step, must be adjusted. In the etch step, the difference in the thickness of the deposited film and the difference in the etch rate are balanced and cancel each other out, achieving total depth uniformity. The microloading effect can then be suppressed by optimizing the duration of film deposition and etching for all pattern widths. Figure 6 shows the result of adjusting the process conditions to control the microloading effect.
Flat-Bottom process
The process for suppressing the microloading effect can also be used for deep Si etching with a wide pattern as shown in Figure 7. This process suppresses not only the microloading effect, but also scallops and round shape at the bottom of trench and hole patterns. It enables anisotropic etching of patterns with widths of several hundred micrometers. However, adjusting process conditions to optimize the depth uniformity of the flat-bottom process is very challenging. Samco has a wealth of knowledge and process libraries for the flat-bottom process and is able to provide our customers with the most suitable deep Si etching processes.
Want to continue reading the Bosch Process Tutorial series?
Process capabilities of Samco's Si DRIE Systems
Samco’s silicon deep reactive ion etching (Si-DRIE) systems utilize both the Bosch and Non-Bosch processes to enable precise fabrication of trenches, holes, and pillars for various device applications. Below are examples of structures fabricated using these techniques:
- Bosch Process for Micro Fabrication
- Non-Bosch Process for through-silicon via (TSV)